{"id":5516,"date":"2026-11-03T06:51:57","date_gmt":"2026-11-02T22:51:57","guid":{"rendered":"https:\/\/www.corvelanmag.com\/?p=5516"},"modified":"2026-11-20T21:46:43","modified_gmt":"2026-11-20T13:46:43","slug":"magnetic-separation-testing-procedure","status":"publish","type":"post","link":"https:\/\/www.corvelanmag.com\/ru\/magnetic-separation-testing-procedure\/","title":{"rendered":"\u0418\u0441\u043f\u044b\u0442\u0430\u043d\u0438\u044f \u043c\u0430\u0433\u043d\u0438\u0442\u043d\u043e\u0439 \u0441\u0435\u043f\u0430\u0440\u0430\u0446\u0438\u0438: \u043f\u043e\u0434\u0433\u043e\u0442\u043e\u0432\u043a\u0430 \u043f\u0440\u043e\u0431 \u0438 \u0441\u0440\u0430\u0432\u043d\u0435\u043d\u0438\u0435 \u0440\u0435\u0437\u0443\u043b\u044c\u0442\u0430\u0442\u043e\u0432"},"content":{"rendered":"\n<style>\n\n.cv-testing{color:#202124;font-family:inherit;font-size:17px;line-height:1.75;overflow-wrap:anywhere}\n.cv-testing section,.cv-testing .cv-intro,.cv-testing .cv-close{box-sizing:border-box;margin:0 0 26px;padding:22px;border:1px solid #dadce0;border-top:3px solid #50545a;border-radius:8px;background:#fff;box-shadow:0 2px 8px #20212408}\n.cv-testing .cv-intro,.cv-testing nav,.cv-testing .cv-close{background:#f7f7f7}\n.cv-testing h2{font-size:27px;line-height:1.3;margin:0 0 18px;color:#202124}\n.cv-testing h3{font-size:21px;line-height:1.4;margin:28px 0 12px;color:#202124}\n.cv-testing p{margin:0 0 16px}.cv-testing p:last-child{margin-bottom:0}\n.cv-testing ul,.cv-testing ol{margin:12px 0 20px;padding-left:25px}.cv-testing li{margin:0 0 10px}\n.cv-testing a{color:#30343b;text-decoration:underline;text-underline-offset:3px}.cv-testing a:hover{text-decoration-thickness:2px}\n.cv-testing a:focus-visible,.cv-testing [tabindex]:focus-visible{outline:3px solid #30343b;outline-offset:4px}\n.cv-testing nav{border:1px solid #dadce0;border-radius:8px;margin:0 0 26px;padding:22px}\n.cv-testing nav a{white-space:normal}.cv-testing section{scroll-margin-top:110px}\n.cv-testing .cv-media{display:block;float:none;clear:both;margin:22px 0 0}\n.cv-testing .cv-media img{display:block;float:none;max-width:100%;height:auto;margin-inline:auto}\n.cv-testing .cv-table{overflow-x:auto;margin:20px 0;border:1px solid #dadce0;border-radius:6px}\n.cv-testing table{width:100%;border-collapse:collapse;font-size:16px;line-height:1.6}\n.cv-testing th,.cv-testing td{padding:12px 14px;text-align:left;vertical-align:top;border-bottom:1px solid #dadce0}\n.cv-testing th{color:#202124;background:#f1f3f4;font-weight:700}.cv-testing tbody tr:last-child td{border-bottom:0}\n@media(max-width:640px){.cv-testing{font-size:16px;line-height:1.7}.cv-testing section,.cv-testing .cv-intro,.cv-testing .cv-close,.cv-testing nav{padding:18px;margin-bottom:20px}.cv-testing h2{font-size:23px}.cv-testing h3{font-size:20px}.cv-testing th,.cv-testing td{padding:10px}.cv-testing table{font-size:15px}}\n.cv-testing .cv-trial-prompt{background:#f7f7f7;padding-block:18px}\n.cv-testing .cv-trial-prompt h2{margin-bottom:8px;font-size:22px}\n.cv-testing .cv-trial-actions{display:flex;flex-wrap:wrap;align-items:stretch;gap:10px}\n.cv-testing a.cv-trial-button{box-sizing:border-box;display:inline-flex;align-items:center;justify-content:center;min-height:44px;padding:8px 14px;border:1px solid #50545a;border-radius:5px;background:#30343b;color:#fff;font-weight:700;line-height:1.4;text-align:center;text-decoration:none}\n.cv-testing a.cv-trial-button-secondary{background:#fff;color:#30343b}\n.cv-testing a.cv-trial-button:hover{background:#4b5058;color:#fff}\n.cv-testing a.cv-trial-button-secondary:hover{background:#eceef0;color:#30343b}\n.cv-testing .cv-trial-brief{background:#f7f7f7}\n.cv-testing .cv-brief-grid{display:grid;grid-template-columns:repeat(2,minmax(0,1fr));gap:12px;margin:16px 0 20px}\n.cv-testing .cv-brief-card{min-width:0;padding:14px 16px;border:1px solid #dadce0;border-radius:6px;background:#fff}\n.cv-testing .cv-brief-card h3{margin:0 0 5px;font-size:18px}\n.cv-testing .cv-brief-card p{margin:0}\n@media(max-width:640px){.cv-testing .cv-trial-prompt h2{font-size:20px}.cv-testing .cv-brief-grid{grid-template-columns:minmax(0,1fr)}.cv-testing .cv-trial-actions{flex-direction:column}.cv-testing .cv-trial-actions a{width:100%}}\n<\/style>\n<div class=\"cv-testing\">\n<div class=\"cv-intro\"><p><strong>A useful magnetic separation testing procedure starts with representative material and a clear product target. Prepare matched test portions, record the separator and feed conditions, collect every output, then compare grade, target recovery and product yield together.<\/strong> Keep the original measurements so another person can repeat the calculations.<\/p>\n<p>A bag of material sticking to a magnet tells you little about the saleable product. The useful question is whether the tested setup gives the quality and recovery you need at a practical feed rate. This guide explains how to prepare the sample, run a fair comparison and read the results.<\/p><\/div>\n<section class=\"cv-trial-prompt\" aria-labelledby=\"trial-prompt-heading\">\n  <h2 id=\"trial-prompt-heading\">Planning a Magnetic Separation Trial?<\/h2>\n  <p>Share your material, what you need to remove or recover, and your normal operating conditions. If you already have test results, include the feed and product measurements, separator settings, and the decision you\u2019re trying to make.<\/p>\n  <div class=\"cv-trial-actions\">\n    <a class=\"cv-trial-button cv-trial-button-secondary\" href=\"#material-test-brief\">See What Information to Prepare<\/a>\n    <a class=\"cv-trial-button\" href=\"https:\/\/www.corvelanmag.com\/contact-us\/\">Discuss Your Material and Test Requirements<\/a>\n  <\/div>\n<\/section>\n<nav aria-label=\"Article contents\"><p><strong>In this guide<\/strong><\/p><ol><li><a href=\"#targets\">What should a magnetic separation test measure?<\/a><\/li><li><a href=\"#samples\">How do you prepare representative samples?<\/a><\/li><li><a href=\"#procedure\">How do you run a fair magnetic separation test?<\/a><\/li><li><a href=\"#calculations\">How do you calculate recovery, grade and mass balance?<\/a><\/li><li><a href=\"#reports\">How should you compare two test reports?<\/a><\/li><li><a href=\"#production\">What should you test before moving to production?<\/a><\/li><li><a href=\"#testing-faq\">Magnetic separation testing FAQs<\/a><\/li><\/ol><\/nav>\n<section id=\"targets\">\n<h2>What should a magnetic separation test measure?<\/h2>\n<p><strong>Measure the result your process needs: valuable material recovered, unwanted material removed, and how much acceptable product remains.<\/strong> Define the target before choosing the test machine or changing its settings.<\/p>\n<div class=\"cv-table\" role=\"region\" tabindex=\"0\" aria-label=\"Your job comparison\"><table><thead><tr><th scope=\"col\">Your job<\/th><th scope=\"col\">Measure first<\/th><th scope=\"col\">Measure alongside it<\/th><\/tr><\/thead><tbody><tr><td>Recover a valuable magnetic mineral<\/td><td>Target mineral or element recovered into the concentrate<\/td><td>Concentrate grade, mass yield and target left in tailings<\/td><\/tr><tr><td>Remove iron-bearing impurities from silica or another industrial mineral<\/td><td>Residual impurity in the saleable product<\/td><td>Product yield and valuable material lost with the reject<\/td><\/tr><tr><td>Recover iron and steel from mixed recycling feed<\/td><td>Recovered mass of the specified iron or steel fraction<\/td><td>Ferrous-product purity, missed target and non-target carryover<\/td><\/tr><\/tbody><\/table><\/div>\n<p><strong>Grade<\/strong> means the content of the component you are measuring, such as total Fe in a concentrate. <strong>Recovery<\/strong> means the share of that component in the feed that reaches the selected product. <strong>Mass yield<\/strong> means the share of total feed mass that reaches that product. A heavy magnetic fraction may contain a lot of unwanted material, so its weight alone is not target recovery.<\/p>\n<p>Write a short test objective. For example: \u201cFind a setting that meets the required concentrate Fe grade while retaining enough feed Fe at the planned dry-solids feed rate.\u201d Put the actual grade, recovery and rate requirements in the test brief. Where several settings meet them, compare product loss and the equipment needed to maintain the result.<\/p>\n<p>Use the same identity throughout the brief and report. Total Fe includes iron in different minerals; it is not automatically magnetite content. For scrap, define whether \u201ctarget\u201d means all ferrous pieces, a size class or a specified alloy. The sample analysis and sorting method must measure that target.<\/p>\n<p>If your trial focuses on recovering iron and steel from mixed scrap or improving the purity of the recovered fraction, see the <a href=\"https:\/\/www.corvelanmag.com\/applications\/scrap-metal-separation\/\">scrap metal separation application guide<\/a>.<\/p>\n<\/section>\n<section id=\"samples\">\n<h2>How do you prepare representative samples?<\/h2>\n<div class=\"cv-media\"><img loading=\"lazy\" src=\"https:\/\/www.corvelanmag.com\/wp-content\/uploads\/2026\/10\/corvelan-sample-workbench-reference-20261030-v1.webp\" alt=\"Sample trays, sieve and scoop on a metal workbench\" width=\"1200\" height=\"900\" loading=\"lazy\" decoding=\"async\" style=\"display:block;max-width:100%;height:auto;object-fit:contain;\"><\/div>\n<p><strong>Collect material that represents the production feed, divide it into matched portions, and preserve the condition you plan to process.<\/strong> Keep a reserve before any drying, crushing or screening changes the sample.<\/p>\n<h3>Collect material across the feed you need to represent<\/h3>\n<p>Define the source first: one batch, a production period, an ore type or a blend. Take increments across that source using a safe sampling point and a method suited to the stream. A scoop from the top of a stockpile can miss settled coarse particles or segregated fines. Do not reach into running equipment to collect a sample.<\/p>\n<p>Record the sample ID, source, collection times, collection method, particle-size range and moisture or slurry condition. If moisture, ore type or contamination changes enough to affect separation, keep those conditions as separate sample groups. A blended \u201caverage\u201d can hide the feed that causes the plant to miss its target.<\/p>\n<h3>Split the sample without picking its best-looking particles<\/h3>\n<p>Use a suitable sample divider to prepare the head-analysis sample, separation-test portions and reserve. For dry, free-flowing material, a correctly sized riffle or rotary splitter can help produce matched portions. The splitter must accept the largest particles without blockage or selective loss.<\/p>\n<p>Coarse metal pieces, wet sticky feed and material that settles quickly need a different sampling arrangement. <a href=\"https:\/\/als-prod-sitecoreai.alsglobal.com\/geochemistry\/sample-preparation\/individual-preparation-procedures\" rel=\"nofollow noopener\" target=\"_blank\">ALS describes both riffle and rotary splitting<\/a>, including the risk of dense native-metal particles segregating during vibratory feeding. Match the preparation method to the material rather than choosing a splitter by convenience.<\/p>\n<p>Label each portion and weigh it. For slurry, use a method that keeps solids suspended and takes representative portions; decanting clear water and scooping settled solids changes the solids distribution. Retain enough material for repeats and for checking an unexpected result.<\/p>\n<h3>Keep separation preparation separate from assay preparation<\/h3>\n<p>Run the separation sample at the planned process particle size and moisture. Pulverize only the analytical split when the chosen assay method requires it. Grinding the entire separation sample can free mineral grains and make the result describe a different process.<\/p>\n<p>If drying, screening, washing or grinding is part of the proposed plant, record that preparation as a test step. Weigh removed size fractions or slimes, and include their target content in the overall result when they leave the circuit. Also keep a record of the as-received material.<\/p>\n<p>Clean preparation equipment between samples. When measuring small iron contamination, discuss possible iron pickup from steel crushers, mills or tools with the laboratory. Use suitable preparation materials and blanks where needed; contamination introduced during preparation can mask the separation result.<\/p>\n<h3>Agree sample quantity from the actual test plan<\/h3>\n<p>There is no single kilogram requirement for every magnetic separation test. Coarse particles, rare contaminants, a wide size range, multiple settings and continuous trials can all increase the amount needed.<\/p>\n<p>Allocate material to head analysis, every planned fresh-feed run, repeats, handling losses and a sealed reserve. Ask the test facility to size those portions for its equipment before dispatch. Send the sample list and relevant safety information, and agree packaging, receiving details and return or disposal arrangements.<\/p>\n<\/section>\n<section id=\"procedure\">\n<h2>How do you run a fair magnetic separation test?<\/h2>\n<p><strong>Use matched fresh-feed portions, hold the agreed conditions steady, and record every deliberate change.<\/strong> Start with a baseline that can be repeated before comparing settings or separator types.<\/p>\n<p>Choose a machine that can test the intended material state and target. Our <a href=\"https:\/\/www.corvelanmag.com\/products\/dry-drum-magnetic-separator\/\">dry drum magnetic separator<\/a> is a candidate for dry, controllable feed with a strongly magnetic target. Our <a href=\"https:\/\/www.corvelanmag.com\/products\/wet-drum-magnetic-separator\/\">wet drum magnetic separator<\/a> handles strongly magnetic material in slurry. A <a href=\"https:\/\/www.corvelanmag.com\/products\/magnetic-roller-separator\/\">high-intensity magnetic roller separator<\/a> is a candidate for dry, liberated, weakly magnetic particles presented in a thin, even layer.<\/p>\n<p>If you\u2019re narrowing down which equipment types to test, use the <a href=\"https:\/\/www.corvelanmag.com\/magnetic-separator-selection-guide\/\">magnetic separator selection guide<\/a> to compare options by material and duty.<\/p>\n<div class=\"cv-table\" role=\"region\" tabindex=\"0\" aria-label=\"Test setup comparison\"><table><thead><tr><th scope=\"col\">Test setup<\/th><th scope=\"col\">Record and control<\/th><\/tr><\/thead><tbody><tr><td>Dry drum<\/td><td>Size distribution, moisture, feed rate, working width, layer depth, drum speed, magnetic configuration and splitter position<\/td><\/tr><tr><td>Wet drum<\/td><td>Dry-solids rate, slurry flow, solids concentration, size distribution, tank arrangement, drum speed, magnetic loading and collection conditions<\/td><\/tr><tr><td>Dry high-intensity roll<\/td><td>Size range, moisture, feed uniformity, layer thickness, belt and roll arrangement, speed, splitter position and number of stages<\/td><\/tr><\/tbody><\/table><\/div>\n<p>Record the actual magnetic configuration. If reporting a field reading, include the instrument, probe orientation, measurement point and gap. Two surface Gauss readings do not make different separator geometries equivalent.<\/p>\n<ol><li><strong>Prepare the run sheet.<\/strong> List sample IDs, settings, run order, measurements and the product limits to be used. Check scale performance and record container tare masses.<\/li><li><strong>Set up safe collection.<\/strong> Identify every product, reject and middlings stream. Middlings are material kept between the main products for further separation. Use separate, labeled containers. Isolate moving equipment before changing mechanical settings or clearing retained material.<\/li><li><strong>Establish the baseline.<\/strong> Feed a matched portion under recorded conditions. In a continuous test, allow the feed and discharge to settle before timed sampling. Keep startup and shutdown material separate, or include them consistently in the batch totals.<\/li><li><strong>Collect all outputs.<\/strong> Measure the feed and each output over the same defined batch or steady sampling period. Account for dust, spills, retained solids and wash-water solids. Keep process water separate from the dry-solids mass calculation.<\/li><li><strong>Compare planned conditions.<\/strong> For a simple first check, change one setting and keep the others fixed. Record actual feed rate rather than only the feeder dial position.<\/li><li><strong>Repeat with fresh matched feed.<\/strong> Keep individual run results. Feeding the previous concentrate through again tests another cleaning stage; it is not an independent repeat of the first pass.<\/li><\/ol>\n<p><a href=\"https:\/\/www.itl.nist.gov\/div898\/handbook\/pri\/section1\/pri14.htm\" rel=\"nofollow noopener\" target=\"_blank\">NIST&#8217;s experiment-planning guidance<\/a> stresses clear objectives, checked measuring devices, raw records and attention to drift. Apply that here by keeping a baseline run and noting surging, buildup, setting changes or sampling interruptions beside the result.<\/p>\n<p>For longer comparisons, group runs by comparable feed batch or test day, then vary the order within those groups where practical. This helps separate a setting effect from a change in feed or operating condition. NIST explains the method in its guidance on <a href=\"https:\/\/www.itl.nist.gov\/div898\/handbook\/pri\/section3\/pri332.htm\" rel=\"nofollow noopener\" target=\"_blank\">randomized block designs<\/a>.<\/p>\n<p>One-setting-at-a-time trials are useful for diagnosis, but settings can interact. A speed that works with a thin feed layer may fail with a deeper one. Where that interaction matters, plan combinations of feed rate, speed or splitter position rather than calling one isolated result the optimum. Keep enough sample to repeat the preferred combination.<\/p>\n<\/section>\n<section id=\"calculations\">\n<h2>How do you calculate recovery, grade and mass balance?<\/h2>\n<p><strong>Use dry-solids masses and assays of the same component on the same basis. Calculate product yield and component recovery separately, then check both mass and component balance.<\/strong> A precise percentage is useful only when its input measurements match.<\/p>\n<h3>Put feed and products on one measurement basis<\/h3>\n<p>For a two-product mineral test, use:<\/p>\n<ul><li><strong>F:<\/strong> dry feed mass; <strong>C:<\/strong> dry concentrate mass; <strong>T:<\/strong> dry tailings mass.<\/li><li><strong>f, c and t:<\/strong> the feed, concentrate and tailings grades of the same measured component.<\/li><li><strong>Grade:<\/strong> component mass divided by dry sample mass, reported as a fraction, percentage or other stated unit.<\/li><\/ul>\n<p>Use one mass unit throughout. If moisture is measured on a wet basis, dry mass = wet mass \u00d7 (1 \u2212 moisture fraction). Thus, 5 kg at 20% wet-basis moisture contains 4 kg of dry solids. Use the measured moisture for each stream; a wet concentrate and a damp tailing rarely contain the same water fraction.<\/p>\n<div class=\"cv-table\" role=\"region\" tabindex=\"0\" aria-label=\"Result comparison\"><table><thead><tr><th scope=\"col\">Result<\/th><th scope=\"col\">Formula<\/th><th scope=\"col\">What it tells you<\/th><\/tr><\/thead><tbody><tr><td>Concentrate mass yield (%)<\/td><td>100 \u00d7 C \/ F<\/td><td>How much total feed mass enters the concentrate<\/td><\/tr><tr><td>Component recovery (%)<\/td><td>100 \u00d7 C \u00d7 c \/ (F \u00d7 f)<\/td><td>How much feed component enters the concentrate<\/td><\/tr><tr><td>Dry-mass closure (%)<\/td><td>100 \u00d7 (C + T) \/ F<\/td><td>Whether the collected dry outputs account for the feed mass<\/td><\/tr><tr><td>Component closure (%)<\/td><td>100 \u00d7 (C \u00d7 c + T \u00d7 t) \/ (F \u00d7 f)<\/td><td>Whether the measured component in both products accounts for that in the feed<\/td><\/tr><\/tbody><\/table><\/div>\n<p>For recovery and component closure, enter grades consistently: all as fractions or all as percentages. To obtain kilograms of component, convert percentage grade to a fraction first. The yield and recovery definitions are also used in this <a href=\"https:\/\/www.mdpi.com\/2673-6489\/5\/2\/21\" rel=\"nofollow noopener\" target=\"_blank\">published laboratory separation study, Section 2.7<\/a>.<\/p>\n<p>Add every output when there are more than two products. Include middlings, removed fines and separately collected losses. Keep measured raw values alongside any reconciled balance; do not silently adjust masses or assays to force closure to 100%.<\/p>\n<h3>Compare two settings with a complete worked example<\/h3>\n<p>Suppose two matched portions each contain <strong>10 kg of dry feed at 20% Fe<\/strong>, or <strong>2 kg of feed Fe<\/strong>. Both tests use the same preparation, feed rate and assay method. For this example, the product must reach at least <strong>58% Fe<\/strong> and recover at least <strong>88% of feed Fe<\/strong>.<\/p>\n<div class=\"cv-table\" role=\"region\" tabindex=\"0\" aria-label=\"Measurement or result comparison\"><table><thead><tr><th scope=\"col\">Measurement or result<\/th><th scope=\"col\">Setting A<\/th><th scope=\"col\">Setting B<\/th><\/tr><\/thead><tbody><tr><td>Dry feed mass and Fe grade<\/td><td>10 kg; 20%<\/td><td>10 kg; 20%<\/td><\/tr><tr><td>Dry concentrate mass and Fe grade<\/td><td>3 kg; 60%<\/td><td>4 kg; 47.5%<\/td><\/tr><tr><td>Dry tailings mass and Fe grade<\/td><td>7 kg; about 2.857%<\/td><td>6 kg; about 1.667%<\/td><\/tr><tr><td>Concentrate mass yield<\/td><td>30%<\/td><td>40%<\/td><\/tr><tr><td>Fe in concentrate<\/td><td>1.8 kg<\/td><td>1.9 kg<\/td><\/tr><tr><td>Fe recovery<\/td><td>90%<\/td><td>95%<\/td><\/tr><tr><td>Dry-mass closure<\/td><td>100%<\/td><td>100%<\/td><\/tr><tr><td>Fe closure, allowing for displayed rounding<\/td><td>About 100%<\/td><td>About 100%<\/td><\/tr><\/tbody><\/table><\/div>\n<p>For A, Fe recovery = 100 \u00d7 (3 \u00d7 0.60) \/ (10 \u00d7 0.20) = <strong>90%<\/strong>. Its tailings contain 0.2 kg Fe, so the calculated tailings grade is 0.2 \/ 7 \u00d7 100 \u2248 <strong>2.857% Fe<\/strong>.<\/p>\n<p><strong>Choose A against the example limits: it meets both grade and recovery.<\/strong> B recovers more Fe but carries more other material into its concentrate. If B needs a cleaning stage to reach 58% Fe, compare the final circuit&#8217;s overall recovery, capacity and product quality with A. Its initial 95% recovery is not the final cleaned-product recovery.<\/p>\n<h3>Distinguish impurity reduction from impurity removal<\/h3>\n<p>Now suppose an iron-removal test treats <strong>10 kg at 0.30% Fe<\/strong> and retains <strong>9.5 kg of saleable product at 0.08% Fe<\/strong>.<\/p>\n<ul><li>Concentration reduction = 100 \u00d7 (0.30 \u2212 0.08) \/ 0.30 \u2248 <strong>73.3%<\/strong>.<\/li><li>Feed Fe = 10 \u00d7 0.003 = <strong>0.030 kg<\/strong>.<\/li><li>Fe left in saleable product = 9.5 \u00d7 0.0008 = <strong>0.0076 kg<\/strong>.<\/li><li>Share of feed Fe outside the saleable product = 100 \u00d7 (0.030 \u2212 0.0076) \/ 0.030 \u2248 <strong>74.7%<\/strong>.<\/li><li>Saleable-product mass yield = 100 \u00d7 9.5 \/ 10 = <strong>95%<\/strong>.<\/li><\/ul>\n<p>The product concentration and product yield answer different questions. To attribute the missing Fe to a captured magnetic reject, weigh and assay that reject and close the full balance. Spilled or retained material also sits outside the saleable product, so it must not be counted automatically as successful magnetic capture.<\/p>\n<h3>Check the balance before ranking performance<\/h3>\n<p>Perfect closure is the conservation target. Actual measurements have uncertainty, so agree acceptable closure and repeatability for the method before testing. The limits should fit the sampling, weighing, moisture and assay methods.<\/p>\n<p>If closure falls outside those limits, investigate retained solids, spills, water corrections, sample labels and analytical results before ranking settings. Dry-mass closure alone is insufficient: all solids can be collected while a poorly split assay sample still gives the wrong Fe balance. If feed component content is zero or unknown, component recovery cannot be calculated from these formulas.<\/p>\n<\/section>\n<section id=\"reports\">\n<h2>How should you compare two test reports?<\/h2>\n<p><strong>First match the feed, preparation, measurement basis and process stages. Then compare quality, recovery, yield and feed rate, using the individual repeat results to judge how stable the difference is.<\/strong> A higher headline recovery can come from an easier sample or a less selective split.<\/p>\n<p>Read both reports against the following points:<\/p>\n<ul><li><strong>Sample identity:<\/strong> same source and representative splits, or a clear explanation of how the feeds differ.<\/li><li><strong>Preparation:<\/strong> size distribution, moisture, grinding, washing and excluded fractions.<\/li><li><strong>Machine and duty:<\/strong> separator type, working width, magnetic configuration, feed presentation and measured operating rate.<\/li><li><strong>Stages:<\/strong> single pass, repeated cleaning, scavenging of tailings, or a complete circuit. Keep each stage&#8217;s products traceable.<\/li><li><strong>Measurements:<\/strong> dry masses, sample locations, assay methods, units, detection limits and the component being reported.<\/li><li><strong>Results:<\/strong> raw run data, product grades, recoveries, yields, both balances and any excluded or interrupted runs.<\/li><\/ul>\n<p>If one facility reports total-Fe recovery and another reports magnetic mass yield, put them in separate columns. Obtain the missing masses and assays before ranking them on recovery. Likewise, convert wet feed rate to dry-solids rate before comparing a slurry test with a dry test.<\/p>\n<h3>Decide whether the difference is repeatable<\/h3>\n<p>Repeat the preferred conditions with fresh matched portions. An assay duplicate checks analysis; a second split checks part of sample preparation; a fresh full separation run checks more of the test procedure. They answer different questions.<\/p>\n<p>Keep the individual values, mean and spread. If the between-setting difference is smaller than the within-setting variation, first stabilize sampling and operation. Use more planned repeats or a suitable statistical analysis before choosing a winner. Do not discard an inconvenient run without recording the event that made it invalid.<\/p>\n<h3>Follow up the result that does not make sense<\/h3>\n<p>If dry mass is missing, inspect collection boundaries, spills and material left in the feeder, tank or piping. If dry mass closes but component balance does not, review head-sample representativeness, product subsampling, labels, moisture correction and assay basis.<\/p>\n<p>For a result close to the product limit, retain sealed feed and product splits. A separate qualified laboratory can reanalyze matched splits with a suitable method. Agree sample IDs and the analysis required before sending them. Reanalysis checks the chemical result; repeating the separation on reserve feed checks whether the process result can be reproduced.<\/p>\n<p>Ask for a corrected report with raw values and the reason for the change. This gives you a record that can be checked independently instead of relying on a photograph or a supplier&#8217;s final percentage.<\/p>\n<\/section>\n<section id=\"production\">\n<h2>What should you test before moving to production?<\/h2>\n<p><strong>Test the preferred setup with normal production material, the required feed rate and the feed conditions that are most likely to cause a miss.<\/strong> Move from a response check to a controlled separation trial, then to continuous testing when flow, loading or equipment buildup affects the decision.<\/p>\n<p>A hand-magnet check or small batch can establish a useful starting point. A continuous trial shows whether the feed stays even, each discharge remains separate, and product quality holds as the machine carries material. The <a href=\"https:\/\/www.gtk.fi\/en\/research-methods\/magnetic-separation\/\" rel=\"nofollow noopener\" target=\"_blank\">Geological Survey of Finland describes both batch laboratory and continuous factory testing<\/a>, reflecting these different test duties.<\/p>\n<p>Use the result to choose the next action:<\/p>\n<div class=\"cv-table\" role=\"region\" tabindex=\"0\" aria-label=\"What the trial shows comparison\"><table><thead><tr><th scope=\"col\">What the trial shows<\/th><th scope=\"col\">What to test next<\/th><\/tr><\/thead><tbody><tr><td>Product meets quality at low rate but misses at the required rate<\/td><td>Feed distribution, layer depth or slurry loading at the required rate; compare suitable working width or parallel capacity<\/td><\/tr><tr><td>Recovery is acceptable but concentrate grade is low<\/td><td>A more selective split or cleaning stage; measure the new final-product recovery and grade<\/td><\/tr><tr><td>Product grade is acceptable but too much target remains in tailings<\/td><td>Tailings size and target response, a less selective setting or a scavenging stage that recovers target from tailings<\/td><\/tr><tr><td>Specially dried or screened feed works, normal feed does not<\/td><td>The actual drying, sizing or feeding step needed, including the mass and target content removed during preparation<\/td><\/tr><tr><td>Repeated runs drift as material builds up<\/td><td>A longer run covering loading and cleaning behavior, with time-linked feed and product samples<\/td><\/tr><\/tbody><\/table><\/div>\n<p>For dry equipment, record dry mass per time, working width and layer condition. For wet equipment, record dry-solids rate as well as slurry flow and solids concentration. Preserve the size distribution and target loading that the machine must handle. Scaling kilograms per hour by drum diameter alone leaves out those conditions.<\/p>\n<p>Select the next trial to resolve the largest remaining decision. If feed lumps are the problem, first test feed preparation. If a mineral is still locked inside another particle, examine liberation before increasing magnetic intensity. If the process needs several stages, carry the balance from original feed to final products, including every reject and middlings stream.<\/p>\n<p>Agree the production acceptance test around the final material range, operating rate, sampling period, product limits and measurement methods. Keep the laboratory report and production results in the same units so the first production run can be compared with the proposed setup.<\/p>\n<\/section>\n<section id=\"decisions-before-ordering\" class=\"cv-trial-decisions\">\n  <h2>What Should You Verify Before Ordering a Magnetic Separator?<\/h2>\n\n  <h3>Recover Magnetite After a Switch to Wet Grinding<\/h3>\n  <p>A dry drum worked when the recovery point was after dry crushing and the feed was dry. If the recovery point moves downstream of wet grinding, the magnetite now reaches the separator in a fine slurry. Evaluate a wet drum for that duty. Before ordering, run a representative sample taken after grinding at the planned slurry flow and solids concentration. Compare concentrate grade, magnetite recovery, and how much magnetite remains in the tailings.<\/p>\n\n  <h3>Meet a Tighter Concentrate Grade Without Losing Too Much Recovery<\/h3>\n  <p>Your current single-pass setting may have met the previous grade and recovery targets. If a buyer raises the minimum grade and repeat runs fall short under the intended feed conditions, compare a more selective setting with adding a cleaning stage. Use matched fresh-feed portions and the same feed rate and assay method. For each option, measure final concentrate grade and overall recovery from the original feed, then check both against your acceptance limits.<\/p>\n\n  <h3>Hold Product Quality at Production Throughput<\/h3>\n  <p>The tested setup may meet the quality target at a low feed rate. If quality drops at the required production rate and the feed layer deepens or slurry loading rises, check feed distribution first. If the result still falls short, evaluate a wider unit or parallel capacity where the layout allows. Verify the proposed setup in a continuous trial using representative feed at the required rate. Take timed feed and product samples and check grade, recovery, and yield as material loads the separator.<\/p>\n<\/section>\n<div class=\"cv-close\"><p><strong>A reliable magnetic separation testing procedure connects the sample to the decision.<\/strong> Keep the feed representative, make the runs comparable, collect and analyze the outputs, and choose a setup that meets quality and recovery at the required rate. Check unusual results through the raw records, retained samples and a repeat of the relevant test.<\/p>\n<\/div>\n<section id=\"material-test-brief\" class=\"cv-trial-brief\" aria-labelledby=\"material-test-brief-heading\">\n  <h2 id=\"material-test-brief-heading\">Prepare Your Material and Test Brief<\/h2>\n  <p>You can start with the information you already have. Tell us what you\u2019d like the trial or a review of your existing results to help you decide.<\/p>\n  <div class=\"cv-brief-grid\">\n    <div class=\"cv-brief-card\">\n      <h3>Material and Objective<\/h3>\n      <p>Material name and source, photos if available, and what you need to remove or recover.<\/p>\n    <\/div>\n    <div class=\"cv-brief-card\">\n      <h3>Feed Conditions<\/h3>\n      <p>Particle size range, moisture for dry feed or solids concentration for slurry if known, and any preparation such as screening or grinding.<\/p>\n    <\/div>\n    <div class=\"cv-brief-card\">\n      <h3>Operating Requirements<\/h3>\n      <p>Normal and peak throughput, where the separator would go in the process, and any equipment already in use at that stage.<\/p>\n    <\/div>\n    <div class=\"cv-brief-card\">\n      <h3>Existing Test Results<\/h3>\n      <p>Feed and product masses, assay results, and separator settings, if available. Include the results for each run you want to compare.<\/p>\n    <\/div>\n  <\/div>\n  <h3>What decision should the results support?<\/h3>\n  <p>Tell us if you\u2019re comparing separator types, checking a product-quality target, investigating losses, or deciding what to test before scaling up.<\/p>\n  <p>If samples are needed, confirm the quantity, preparation, receiving instructions, and test scope before shipping.<\/p>\n  <div class=\"cv-trial-actions\">\n    <a class=\"cv-trial-button\" href=\"https:\/\/www.corvelanmag.com\/contact-us\/\">Discuss Your Material and Test Requirements<\/a>\n  <\/div>\n<\/section>\n<section id=\"testing-faq\" class=\"faq\"><h2>Magnetic separation testing FAQs<\/h2>\n<h3>Is a small bag enough when the feed contains occasional large iron pieces?<\/h3>\n<p><strong>It may be enough for an initial response check, but it can easily miss rare, large contaminants.<\/strong> Tell the test facility the largest target size, how often it appears and the production volume it represents. Plan enough representative material or a separate controlled challenge test. Keep deliberately added test pieces identified; their capture result should not be reported as the natural feed&#8217;s recovery.<\/p>\n<h3>Can I use a hand magnet instead of a laboratory separator?<\/h3>\n<p><strong>Use a hand magnet to screen magnetic response, then use a controlled separator trial for a flow or product-quality decision.<\/strong> A slow hand pass changes the exposure and presentation compared with moving feed. Record the sample condition and what was attracted so the next test can use a suitable separator and measured outputs.<\/p>\n<h3>Does total-Fe recovery show magnetite recovery?<\/h3>\n<p><strong>Only if the measurements establish how the reported Fe relates to magnetite in that material.<\/strong> Total Fe can include other iron-bearing minerals. If magnetite recovery is the objective, use suitable mineralogical or magnetite-specific measurements on feed and products, with the laboratory&#8217;s stated method. Label total-Fe recovery separately.<\/p>\n<h3>Can a three-pass result be compared with a single-pass result?<\/h3>\n<p><strong>Compare them as different process arrangements, using original feed and final products as the common basis.<\/strong> Multiply the stage recoveries only when each stage&#8217;s recovery is defined relative to the component entering that stage. For a simple sequence with no recycle, 90% followed by 95% retains 85.5% of the original component, not 95%. Recycle circuits require a full stream balance.<\/p>\n<h3>Should a result below the detection limit be entered as zero?<\/h3>\n<p><strong>No. Keep the reported limit and use it as a bound when the calculation allows.<\/strong> For example, a dry product reported as less than 50 mg\/kg Fe contains less than 0.05 kg Fe per tonne. Use the same analyte, units and sample basis in the feed result. If the required product limit is below the method&#8217;s reporting capability, use a more sensitive suitable method before deciding acceptance.<\/p><\/section>\n<script type=\"application\/ld+json\">\n{\n  \"@context\": \"https:\/\/schema.org\",\n  \"@type\": \"FAQPage\",\n  \"mainEntity\": [\n    {\n      \"@type\": \"Question\",\n      \"name\": \"Is a small bag enough when the feed contains occasional large iron pieces?\",\n      \"acceptedAnswer\": {\n        \"@type\": \"Answer\",\n        \"text\": \"It may be enough for an initial response check, but it can easily miss rare, large contaminants. Tell the test facility the largest target size, how often it appears and the production volume it represents. Plan enough representative material or a separate controlled challenge test. Keep deliberately added test pieces identified; their capture result should not be reported as the natural feed's recovery.\"\n      }\n    },\n    {\n      \"@type\": \"Question\",\n      \"name\": \"Can I use a hand magnet instead of a laboratory separator?\",\n      \"acceptedAnswer\": {\n        \"@type\": \"Answer\",\n        \"text\": \"Use a hand magnet to screen magnetic response, then use a controlled separator trial for a flow or product-quality decision. A slow hand pass changes the exposure and presentation compared with moving feed. Record the sample condition and what was attracted so the next test can use a suitable separator and measured outputs.\"\n      }\n    },\n    {\n      \"@type\": \"Question\",\n      \"name\": \"Does total-Fe recovery show magnetite recovery?\",\n      \"acceptedAnswer\": {\n        \"@type\": \"Answer\",\n        \"text\": \"Only if the measurements establish how the reported Fe relates to magnetite in that material. Total Fe can include other iron-bearing minerals. If magnetite recovery is the objective, use suitable mineralogical or magnetite-specific measurements on feed and products, with the laboratory's stated method. Label total-Fe recovery separately.\"\n      }\n    },\n    {\n      \"@type\": \"Question\",\n      \"name\": \"Can a three-pass result be compared with a single-pass result?\",\n      \"acceptedAnswer\": {\n        \"@type\": \"Answer\",\n        \"text\": \"Compare them as different process arrangements, using original feed and final products as the common basis. Multiply the stage recoveries only when each stage's recovery is defined relative to the component entering that stage. For a simple sequence with no recycle, 90% followed by 95% retains 85.5% of the original component, not 95%. Recycle circuits require a full stream balance.\"\n      }\n    },\n    {\n      \"@type\": \"Question\",\n      \"name\": \"Should a result below the detection limit be entered as zero?\",\n      \"acceptedAnswer\": {\n        \"@type\": \"Answer\",\n        \"text\": \"No. Keep the reported limit and use it as a bound when the calculation allows. For example, a dry product reported as less than 50 mg\/kg Fe contains less than 0.05 kg Fe per tonne. Use the same analyte, units and sample basis in the feed result. If the required product limit is below the method's reporting capability, use a more sensitive suitable method before deciding acceptance.\"\n      }\n    }\n  ]\n}\n<\/script>\n<\/div>\n","protected":false},"excerpt":{"rendered":"<p>A useful magnetic separation testing procedure starts with representative material and a clear product target. Prepare matched test portions, record the separator and feed conditions, collect every output, then compare grade, target recovery and product yield together. Keep the original measurements so another person can repeat the calculations. A bag of material sticking to a [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":5623,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_acf_changed":false,"footnotes":""},"categories":[1],"tags":[],"class_list":["post-5516","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-blog"],"acf":[],"_links":{"self":[{"href":"https:\/\/www.corvelanmag.com\/ru\/wp-json\/wp\/v2\/posts\/5516","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.corvelanmag.com\/ru\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/www.corvelanmag.com\/ru\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/www.corvelanmag.com\/ru\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/www.corvelanmag.com\/ru\/wp-json\/wp\/v2\/comments?post=5516"}],"version-history":[{"count":2,"href":"https:\/\/www.corvelanmag.com\/ru\/wp-json\/wp\/v2\/posts\/5516\/revisions"}],"predecessor-version":[{"id":6217,"href":"https:\/\/www.corvelanmag.com\/ru\/wp-json\/wp\/v2\/posts\/5516\/revisions\/6217"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/www.corvelanmag.com\/ru\/wp-json\/wp\/v2\/media\/5623"}],"wp:attachment":[{"href":"https:\/\/www.corvelanmag.com\/ru\/wp-json\/wp\/v2\/media?parent=5516"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/www.corvelanmag.com\/ru\/wp-json\/wp\/v2\/categories?post=5516"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/www.corvelanmag.com\/ru\/wp-json\/wp\/v2\/tags?post=5516"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}